Kategorie: filling technology

Many problems occur in practice when forming and filling film packaging. Here the spectrum ranges from cracks, leaky sealed seams to poor production performance. we help to avoid errors or to detect them.

  • When packaging leaks: How to properly test seal strength and package integrity

    When packaging leaks: How to properly test seal strength and package integrity

    When food, pharmaceutical, or cosmetics packaging on retail shelves suddenly “draws air,” the protective gas escapes, liquids leak out, or the product spoils long before the best-before date (BBD) is reached, the big search for the cause usually begins. Frequently, initial suspicion immediately falls on the barrier of the film: “The oxygen barrier is not sufficient!” However, after more than 30 years of laboratory practice at Innoform Testservice and countless damage analyses, I can assure you: In the vast majority of cases, it is not the film web that is the problem – but the heat seal.

    Around 90% of all flexible consumer packaging today is thermally sealed using heat contact processes. The heat seal is the structural Achilles’ heel of any flexible packaging. Exactly there, material properties, machine settings, tool geometries, and the product to be filled meet within fractions of a second. In this detailed technical article, based on scientific market studies (including those by the OFI in Vienna and Fraunhofer IVV / IVLV), our seminar documents, and our accredited testing practice, I will show you how many film packagings actually suffer from sealing problems, why tiny capillaries destroy any high barrier, and how you can reliably avoid typical leaks through clever testing and sound know-how.


    How Many Film Packagings Leak Due to Sealing Problems? A Look at the OFI Study and the Market

    In our seminars, I like to start by asking the provocative question: “What percentage of modified atmosphere or vacuum packaging on supermarket shelves do you think is actually not as tight as the brand owner believes?” The answers from participants usually range from a cautious 0.1 to 0.5 percent – after all, modern packaging lines are highly automated. However, scientific data paints a significantly more unvarnished picture.

    The Well-Known Market Study by OFI in Vienna

    Particularly insightful in this regard is a comprehensive study by the Austrian Research Institute for Chemistry and Technology (OFI) in Vienna (led by Dr. Michael Washüttl, Prof. Manfred Tacker, and Birgit Tauschitz). OFI examined a total of over 1,600 food products packaged under modified atmosphere (MAP – Modified Atmosphere Packaging) from regular retail in the DACH region – including meat and sausage products, cheese, fish, baked goods, and convenience products. In addition, a specific sample of 386 MAP packagings in German retail was examined in detail.

    The result caused a stir throughout the entire packaging industry:

    • Only 56% of all examined MAP packages in retail exhibited an optimal protective gas atmosphere.
    • approx. 33% up to 44% of the packages – and in the German retail sample even almost 50% – showed significant deficiencies in the gas mixture or did not fulfill their purpose of extending shelf life as intended.
    • As main causes, alongside an incorrectly designed film barrier and interactions between the filled product and test gas, the Viennese researchers primarily identified leaks due to defective heat seals: unsuitable sealing tools, misadjusted or incorrectly displaying temperature sensors on the sealing jaws, mechanical overstressing during packaging, as well as product contamination in the seal area.

    Supplementary Studies by WRAP and IVLV / Fraunhofer IVV

    These findings line up seamlessly with further international surveys. A widely cited British study by the organization WRAP (“Seal integrity and the impact on food waste”, Dudbridge & Turner) as well as the IVLV Guideline No. 114 from the research project EVOCOSEAL (Fraunhofer IVV in cooperation with the Universities of Hasselt and KU Leuven) impressively show:

    • In 58% of all cases of defective packaging, contamination of the heat seal (by product splashes, fats, dusts, or condensate) is the primary cause of package failure.
    • Depending on film type and contamination, heat seal strength can drop by up to 88% due to product residues in the seal area.

    Even though these studies were conducted some years ago, the trend remains unbroken today. Sealing problems are still the main cause of leaks in flexible packaging today.

    My Practical Estimate: How Many Packages Are Really Affected Today?

    Naturally, inline quality control has evolved since the first OFI surveys. Obvious “bursts” or completely open seals that are immediately noticed on the filling line usually range between 0.1 and 1% in well-managed operations. But that is only half the truth – because a large portion of critical leaks consists of micro-leaks (capillaries with diameters of 10 to 50 µm) in the fold transition or a pre-damaged hot tack, which often remains undetected during a quick spot check in a water bath or only opens during transport due to pressure and vibration stress.

    When we combine the findings of OFI Vienna, Fraunhofer/IVLV research, and our ongoing laboratory tests at Innoform Testservice, my realistic estimate for today’s market is:

    • 70 to 80% of all real packaging leaks do not occur in the undamaged film area, but directly in or immediately adjacent to the heat seal (seal edges, gussets, 2-/4-layer transitions).
    • Across all flexible film packagings on the market, an estimated 3 to 8% of all packages exhibit avoidable heat seal weak points or micro-leaks.
    • For sensitive MAP packaging, vacuum packaging, liquid and powder products, as well as lines newly converted to mono-materials or paper laminates, the rate of non-optimally sealed joints in practice is often even 5 to 15%.

    “Barrier begins where tightness ends. Before philosophizing about permeation, everything must first be leak-tight.”


    Barrier vs. Tightness: Why a Single 25 µm Hole Renders Any High-Barrier Film Packaging Useless

    To understand why even the smallest sealing defects have such dramatic consequences for product protection, it is worth looking at a simple calculation example that I regularly present in our seminar “Leakage testing, sealing and processing of barrier film packaging (Barrier Films Part 4)”.

    Imagine a classic high-barrier pouch with a surface area of 375 cm², made from a metallized laminate (PET-BO met. 12 µm / PE 90 µm). The oxygen transmission rate (OTR) of this intact barrier film is an excellent 0.3 cm³/(m² · d · bar):

    • Oxygen ingress through permeation (intact film area): Across the entire pouch surface of 375 cm², under a pure oxygen gradient, only 0.011 cm³ of oxygen per day and package diffuses through the material.
    • Oxygen ingress through a single micro-leak in the heat seal: Now let us assume that in the 10 mm wide heat seal there is a single continuous capillary (“cannula”) with a diameter of only 25 µm (half as thin as a human hair!) due to a tiny fold or dust particle. Through this single micro-channel alone, around 0.052 cm³ of gas flows into the package per day.

    In plain English, this means: A single 25 µm capillary in the heat seal allows almost five times as much oxygen into the packaging as the entire high-barrier film combined! And if the pore diameter is 50 µm, the gas ingress multiplies drastically once again. So anyone spending a lot of money on EVOH, SiOx, AlOx, or aluminum barriers without having their heat seals under control is throwing money out the window.

    “How Tight Is Tight?” – Typical Defect Points and Leak Rates

    Absolute leak tightness in a physical sense does not exist – what matters is always which defect size becomes critical for your specific product. The following overview (based on guide values from the Fraunhofer Institute IVV and leak testing technology) helps with practical categorization:

    Everyday requirementCritical pore size / capillary diameterTypical leak rate (guide value)Practical example & risk
    Sifting-proof / Insect-proofapprox. 100 – 200 µm> 10⁻¹ mbar·l/sSugar, flour, rice; protection against stored product pests
    Dust-proofapprox. 25 – 30 µmapprox. 10⁻¹ to 10⁻² mbar·l/sFine powders, spices, cocoa powder
    Water vapor-tightapprox. 20 – 25 µmapprox. 10⁻² mbar·l/sDry products, crackers, milk powder clumping
    Liquid-tight (droplets)approx. 15 – 20 µmapprox. 10⁻² mbar·l/sSoups, sauces, pet food, wet wipes
    Vapor-tight (“sweating”)approx. 10 – 15 µmapprox. 10⁻³ mbar·l/sLoss of aroma, drying out during storage
    Gas-tight & bacteria-proofapprox. 5 – 10 µmapprox. 10⁻⁴ mbar·l/sMAP packages, vacuum packaging, medical devices

    The 5 typical causes of leaking heat seals – and how to avoid them

    When customers from the food, pharmaceutical, or consumer goods industries send rejected pouches or trays to our Oldenburg laboratory, we repeatedly encounter five recurring failure patterns in failure analysis. The good news: every single one of these problems can be reliably eliminated with the right material selection and targeted testing.

    Laboratory heat sealer at Innoform Testservice testing seal strength and package integrity of flexible packaging with overview of standards DIN 55529, ASTM F 1921, DIN EN 868-5 and ASTM D 3078
    Systematic root-cause analysis at Innoform Testservice: Combining seal strength curves (DIN 55529), hot-tack testing (ASTM F 1921), dye penetration (DIN EN 868-5) and vacuum leak testing (ASTM D 3078) reliably detects micro-capillaries and gusset defects.

    1. Contamination in the sealing area (“Sealing through contamination”)

    When filling pouches and trays, cocoa powder, ground coffee, milk powder, or grated cheese swirl up; with wet products, marinades, fats, cooking oils, or condensation splash onto the sealing rim. If this product gets between the sealing jaws, it acts as a release layer and prevents the interdiffusion (entanglement) of the molten polymer chains.

    How to avoid this error: In addition to optimized product dosing and extraction, the sealing medium is key here. While simple standard PE-LD or BOPP quickly reaches its limits when contaminated, low-melting metallocene polyethylenes (mLLDPE), ethylene copolymers (such as EVA), or ionomers (known, for example, as Surlyn®) can flow around dust particles and extremely fine grease films much better due to their low melt viscosity and still seal tightly.

    2. The critical 2-to-4-layer step (side gussets, overlaps, and gusset transitions)

    Take a close look at a typical flowpack or stand-up pouch (Doypack): where the longitudinal seal (fin seal) or the side gusset runs into the cross seal, the material thickness abruptly jumps from two layers to four layers. Exactly at this edge, a small wedge-shaped cavity is formed – the so-called gusset transition (“Zwickel”).

    If the sealing layer is designed too thin (e.g., only a few micrometers of heat-sealable coex-PP) or if the sealing jaws are rigid and incorrectly profiled, the molten polymer volume is simply insufficient to “flood” this step. A continuous capillary channel of 20 to 100 µm remains open.

    How to avoid this error: The thickness and flowability of the sealing layer must always be matched to the total thickness of the laminate and the step height. Using a microtome section under a light microscope combined with a dye penetration test according to DIN 55508-2, we can visualize in the laboratory within a very short time whether the gusset area is filled cleanly or whether polymer mass is missing.

    3. Insufficient hot tack strength (hot tack failure)

    On high-speed vertical form-fill-seal machines (VFFS), the following happens: the cross jaws seal the bottom seam, open, and just milliseconds later, the heavy filling product (e.g., 500 g of nuts, frozen vegetables, or washing powder) drops from the filling tube directly into the still hot, molten heat seal. At the same time, the film draw-down pulls on the seam.

    If the sealing layer has a weak hot tack (hot seal strength) in this hot temperature window, the melt is partially pulled apart. Fine threads, micro-caverns, or local cracks form. The tricky part: when you test the cooled pouch later in a standard tensile test, the seam still appears strong – but due to the micro-channels formed while hot, the pouch is already leaking!

    How to avoid this error: For fast FFS processes, never rely solely on cold heat seal strength. Have a complete hot tack curve recorded according to DIN 55571-2 or ASTM F 1921. It shows exactly at which sealing temperature the material offers the highest resistance in the hot state.

    4. Narrowed sealing windows due to mono-materials and paper laminates (PPWR effect)

    In the past, classic composite films such as PET/PE or OPA/PE were extremely forgiving: the outer PET or PA layer melted only beyond 220 to 250 °C, while the inner PE layer sealed starting at 105 °C. Machine operators enjoyed a comfortable sealing window of 30 to 50 °C. If the seal didn’t hold, you simply increased the machine temperature by 15 degrees – and it ran smoothly.

    With the European Packaging and Packaging Waste Regulation (PPWR) and the shift towards recyclable all-PE or all-PP mono-materials as well as fiber-based barrier papers with wafer-thin dispersion sealing coatings, this picture has completely changed:

    • With polyolefin mono-materials, the melting points of the outer layer (e.g., oriented BOPE or BOPP) and the inner layer (sealing PE or sealing PP) are close together. If sealed too hot, the outer film shrinks, the seam warps, or the liquid polymer is squeezed away at the sealing jaw edge – resulting in a thin spot and a classic seal edge break.
    • With paper laminates, the paper acts as a thermal insulator (poor heat transfer), while the internal dispersion coating is often only a few grams per square meter thin and can barely compensate for irregularities in the paper fibers.
    Sealing curve from an Innoform test report comparing two film samples
    Example from an Innoform test report: Comparing the sealing curves of two film batches (Sample 1 vs. Sample 2) immediately reveals if the seal initiation temperature (SIT) has shifted upwards by 10 to 15 °C.

    How to avoid this error: As the diagram from one of our sample laboratory reports shows, even a slight formulation change during coextrusion (e.g., a lower proportion of low-melting plastomer in the PE blend) can shift the seal initiation temperature (SIT) upwards by 10 to 15 °C. Combining a laboratory sealing curve (DIN 55529), DSC melting point analysis, and FTIR spectroscopy allows us to determine beyond doubt whether the material deviated or whether the temperature distribution of your sealing jaws needs to be readjusted.

    5. The conflict of objectives between seal integrity and easy opening (peel seals)

    Consumers want packaging that can be opened smoothly by hand without scissors (easy-peel) – at the same time, quality assurance demands absolute seal integrity throughout the entire logistics process. A widespread misconception is: “A peel seal of 4 N/15 mm is less tight than a solid weld seam of 40 N/15 mm.”

    Physically, this is not true: as long as the sealing layer is completely sealed through, a peel seal (whether interfacial peel, cohesive peel via incompatible blends such as polybutene-1, or burst/tear peel) is just as gas-tight and liquid-tight as a permanent weld seam. It only becomes critical when external forces – such as the re-tensioning of a vacuum pack, internal pressure increases during truck transport over an Alpine pass, or impacts in the shipping carton – exceed the initial tear force of the peel seal and the seam partially migrates open.

    How to avoid this error: In addition to the pure tensile strength of strip samples, also test the actual opening forces on the complete package in accordance with DIN 55409-1 (flexible packaging materials) or DIN 55409-2 (rigid trays) and specifically adapt the sealing jaw contour (e.g. round profile for smooth initiation) to your peel system.


    Testing correctly at Innoform Testservice: Systematically securing heat seal strength and seal integrity

    In our testing laboratory in Oldenburg, accredited according to DIN EN ISO/IEC 17025 (DAkkS), we strictly distinguish between two complementary testing pillars: mechanical seal strength tests (How high is the holding force and how wide is the process window?) and physical seal integrity / leak tests (Are there continuous channels or pores?). Both aspects are inextricably linked for a clean packaging specification.

    Pillar 1: Testing heat seal strength, seal curves, and hot tack

    During the mechanical testing of heat seals, a sample strip exactly 15 mm wide is punched out perpendicular to the seal seam and pulled apart in a tensile testing machine at a defined speed. But beware: anyone looking only at the bare numerical value in N/15 mm in the test report often overlooks the most important thing!

    “Force values alone are not enough – the failure mode tells the truth.”

    That is why at Innoform we always document the failure mode / fracture pattern for every heat seal strength measurement:

    • Clean peeling (separation of the seal layer): Desirable for easy-opening packaging; in the case of permanent seals, however, it indicates a sealing temperature that is too low (cold seal).
    • Break directly at the seal edge (seal edge break): A typical sign of excessively high sealing temperature or sealing pressure – the sealing layer was squeezed and weakened at the jaw edge.
    • Laminate delamination: The seal seam holds stronger than the lamination between the individual layers – the film splits within the laminate (indication of insufficient interlayer adhesion or an unsuitable laminating adhesive).
    • Elongation / break in the unsealed film strip: The seal seam is stronger than the base material itself (true weld seal).
    Test method at Innoform TestserviceStandard / BasisMeasured parameter & temperature rangeTypical practical benefit
    Heat seal strength (strip tensile test)DIN 55529, ASTM F 88 / F 88M, DIN EN 868-5 App. DMaximum force / profile in N/15 mm (-40 °C to +120 °C) incl. failure modeQuality control of manufactured pouches, medical packaging & trays; testing under deep-freeze or pasteurisation conditions
    Seal curves on the laboratory heat sealerDIN 55529, ASTM F 88Heat seal strength over temperature, time & pressure (e.g. 80 – 220 °C)Determination of seal initiation temperature (SIT) and optimal sealing window; comparison of new mono-materials with reference films
    Hot tack testing (hot seal strength)DIN 55571-2, ASTM F 1921Maximum holding force of the still hot seal in N/15 mm directly after jaw openingEssential for fast v-FFS and h-FFS form-fill-seal machines as well as heavy, bulk or deep-frozen products
    Opening forces of peelable packagesDIN 55409-1 (flexible), DIN 55409-2 (rigid)Tear initiation force and propagation force in N on the original packagePractical evaluation of opening behavior (easy opening) from a consumer perspective
    Seal quality of PE heavy-duty bags & paperDIN 55529, GKV Test Sheets I–IV, DIN EN 868-4Seal strength, fiber tear & seal qualitySecuring heavy-duty bags, industrial pouches, and sterilizable paper-film packaging

    Pillar 2: Overview of seal integrity testing and leak detection

    A high heat seal strength in the strip tensile test does not prove that no microscopic capillary has remained open in the 2-/4-layer gusset. Therefore, we combine strength testing in our test portfolio for heat seal strength & seal integrity with targeted leak detection and seal integrity testing:

    Seal integrity / leak test methodStandard / Test specificationDetection limit (approx.)Working principle & ideal field of application
    Test gas method (forming gas N₂/H₂)IVLV Guideline No. 102< 10 µm (gas-tight)Filling with a hydrogen-nitrogen mixture and highly sensitive H₂ sniffer probe; non-destructive localization of minute gas leaks on MAP and vacuum packaging
    Dye penetration test with methylene blueDIN 55508-2approx. 10 – 20 µmAlcohol solution with low surface tension creeps even into the finest seal capillaries and gussets, staining defects in contrasting blue
    Dye penetration testing (Rhodamine B / aqueous)ASTM F 1929approx. 15 – 50 µmInternational standard (esp. pharma/medical) for detecting channels in transparent and opaque heat seals
    Penetrating oil test & original product testingIn-house method PV036approx. 10 – 20 µmSpecial test for oil- and fat-containing products as well as for detecting micro-pinholes after flex-cracking strain (Gelboflex)
    Vacuum chamber / water bath (bubble emission test)Standard laboratory method (DIN EN ISO 11607 / ASTM D 3078)approx. 15 – 30 µmSubmerging the closed package under defined vacuum; escaping gas bubbles immediately reveal the exact location of the leak
    Light table & copper depositionDIN EN 546-4, FhG Leaflet 29 Sheet 1from 20 µm (optical) or micro-pinholesTesting aluminium foils and aluminium laminates for pinholes, flex cracks, and corrosion defects

    Practical checklist: How to permanently eliminate complaints caused by poor heat seals

    From our daily consulting practice, five specific rules have proven effective in helping film manufacturers, converters, and packers drastically reduce their defect rates:

    1. Specify performance instead of just film thickness: Include the seal initiation temperature (SIT), the sealing window in °C, the required heat seal strength in N/15 mm (incl. desired failure mode!), and, for fast form-fill-seal processes, the minimum hot tack bindingly in your film specification.
    2. Systematically store retained samples: Set aside an unprinted or unsealed retained sample from a film batch proven to run perfectly. If machine malfunctions occur later, a direct comparison between good and bad samples in the laboratory can clarify within a few days what has changed.
    3. Test in the laboratory before switching to mono-materials: Do not go “flying blind” onto the production line with new all-PE, all-PP, or paper laminates. A seal and hot tack curve recorded in advance in the laboratory saves expensive machine downtime and tonnes of scrap.
    4. Regularly inspect sealing jaws thermographically and mechanically: As the OFI study showed, the digital display on the control cabinet often does not match the actual surface temperature of the sealing jaw. Check temperature profiles and pressure distribution (e.g. via carbon paper or pressure-sensitive film impressions) regularly, especially in the area of the 2-/4-layer step-down.
    5. Test seal integrity using the correct method: A brief press on the pouch by hand or an unspecific water bath test is often insufficient for MAP and high-barrier packages. For critical products, use the dye penetration test according to DIN 55508-2 or the test gas method according to IVLV Guideline 102.

    Knowledge protects against failure costs: Our matching Innoform seminars

    Good test results only unfold their full value when procurement, quality assurance, packaging development, and machine operators speak the same technical language. If you and your team would like to dive deeper into the interrelationships between polymer structure, sealing technology, and testing methodology, I recommend our practical web seminars and courses at Innoform Coaching:


    Frequently asked questions on heat seal strength and leak testing (FAQ)

    Why is packaging sometimes leaky despite high heat seal strength in N/15 mm?

    Heat seal strength according to DIN 55529 or ASTM F 88 measures the mechanical holding force on a 15 mm wide strip of the cooled seal. However, leaks often occur locally – for example due to a fine capillary (10–30 µm) at the 2-to-4-layer transition (side gusset/fold), individual product particles in the seal, or a brief opening of the still hot seal due to insufficient hot tack strength. Therefore, strength testing should always be supplemented by targeted leak testing (e.g., methylene blue test according to DIN 55508-2 or test gas testing).

    According to studies, how many modified atmosphere packages (MAP) on the market are defective?

    In the well-known market study by the Austrian Research Institute for Chemistry and Technology (OFI) in Vienna analyzing over 1,600 MAP packages in German-speaking countries, only 56% exhibited an optimal protective gas atmosphere; around one third to 44% (and nearly 50% in a German retail sample of 386 packages) showed defects. Supplementary studies (WRAP, Fraunhofer IVV / IVLV Leaflet 114) demonstrate that in 58% of defective package cases, a contaminated seal is the primary cause. In current practice, it can be assumed that 70 to 80% of all real packaging leaks occur in or directly at the heat seal.

    Which test method detects even the smallest micro-leaks in heat seals?

    For directly visualizing the finest channels in the heat seal down to approx. 10–20 µm, dye penetration testing with methylene blue solution according to DIN 55508-2 (or ASTM F 1929 with aqueous dye solution) is ideal. If closed packages need to be non-destructively tested for gas tightness (flaws < 10 µm), the test gas method using forming gas (hydrogen/nitrogen) and a sensitive hydrogen probe according to IVLV Leaflet No. 102 is the method of choice.

    When should a hot tack test be conducted in addition to the seal curve?

    A hot tack test according to DIN 55571-2 or ASTM F 1921 is indispensable whenever the heat seal is subjected to mechanical stress while still hot and incompletely cooled. This applies above all to high-speed vertical and horizontal form-fill-seal machines (v-FFS / h-FFS), heavy or sharp-edged filled goods, and the transition from classic PET/PE laminates to mono-materials (PE, PP) or barrier papers.


    My Conclusion: In case of damage, let analytics do the talking!

    Leaky packages are not an inevitable fate – and certainly no reason for weeks of playing the blame game between film supplier and packager. Whether a seal fails due to product contamination, a narrow sealing window with a new mono-material, insufficient hot tack, or an open gusset at the 2-to-4-layer transition can now be clarified in the lab quickly, objectively, and in compliance with standards.

    My practical advice is therefore: Specifying is better than philosophizing. And if things get stuck on the line or packages leak air in retail: don’t just blindly adjust the sealing temperature, but send us your good and defective samples to our laboratory in Oldenburg. We test heat seal strength and leak tightness accredited from a single source and provide you with results that allow you to operate safely in production again right away.

    Yours, Karsten Schröder
    Innoform Testservice – Your accredited testing laboratory for flexible packaging

    References, Standards and Further Reading

    • Washüttl, M.; Tacker, M.; Tauschitz, B. (OFI – Austrian Research Institute for Chemistry and Technology, Vienna): Market study on the quality and seal integrity of over 1,600 food products packaged under modified atmosphere (MAP) in retail across the DACH region (incl. a subsample of 386 MAP packages in German retail).
    • Dudbridge, M.; Turner, R. (WRAP – Waste & Resources Action Programme, Banbury / University of Lincoln): Seal integrity and the impact on food waste, Project Code RBC521-001.
    • Industrievereinigung für Lebensmitteltechnologie und Verpackung e. V. (IVLV) / Fraunhofer IVV, Freising / UHasselt / KU Leuven: IVLV Code of Practice No. 114 – Prevention of heat seal defects caused by contamination in the sealing area (CORNET Research Project EVOCOSEAL), as well as IVLV Code of Practice No. 102 – Tightness testing of flexible food packaging using test gas methods.
    • DIN 55529: Packaging – Determining the sealed-seam strength of sealings made of flexible packaging material; ASTM F 88 / F 88M: Standard Test Method for Seal Strength of Flexible Barrier Materials; DIN EN 868-4 & DIN EN 868-5: Packaging for terminally sterilized medical devices.
    • DIN 55571-2 & ASTM F 1921 / F 1921M: Standard Test Methods for Hot Seal Strength (Hot Tack) of Thermoplastic Polymers and Blends Comprising the Sealing Surfaces of Flexible Webs; DIN 55409-1 & DIN 55409-2: Packaging – Determination of opening forces of peelable packaging.
    • DIN 55508-2: Packaging test – Leak testing on flexible packaging – Part 2: Dye penetration test (methylene blue method); ASTM F 1929: Standard Test Method for Detecting Seal Leaks in Porous Medical Packaging by Dye Penetration; ASTM D 3078: Standard Test Method for Determination of Leaks in Flexible Packaging by Bubble Emission; DIN EN ISO 11607-1.
    • Schröder, K. (Innoform Coaching & Innoform GmbH Testservice, Oldenburg): Seminar documentation “Leakage testing, sealing and processing of barrier film packaging – Barrier films Part 4 (BVd)” and “Fundamentals of packaging films (Parts C & G)”.
  • When Packaging Leaks: Testing Seal Strength and Leak Tightness Properly

    When Packaging Leaks: Testing Seal Strength and Leak Tightness Properly

    When a food, pharmaceutical or cosmetics package suddenly “draws air” on the retail shelf, the modified atmosphere escapes, liquids leak out or the product spoils long before its best-before date, the search for the cause usually begins in earnest. Very often, suspicion falls immediately on the barrier of the film: “The oxygen barrier isn’t good enough!” But after more than 30 years of laboratory practice at Innoform Testservice and countless failure analyses, I can assure you that in the vast majority of cases, the film web is not the problem – the seal is.

    Around 90% of all flexible consumer packaging today is heat-sealed using thermal contact processes. The seal is the structural Achilles’ heel of every flexible package. This is exactly where material properties, machine settings, tool geometries and the product being filled come together within fractions of a second. In this detailed technical article, drawing on scientific market studies (including those by OFI in Vienna and Fraunhofer IVV / IVLV), our seminar materials and our accredited testing practice, I will show you how many film packages actually suffer from sealing problems, why tiny capillaries undermine even the best high barrier, and how you can reliably avoid typical leaks through smart testing and sound know-how.


    How many film packages leak because of sealing problems? A look at the OFI study and the market

    At the start of our seminars, I like to ask a provocative question: “How many modified atmosphere or vacuum packs on the supermarket shelf do you think are not actually as leak-tight as the brand owner believes?” Participants’ answers usually lie at a cautious 0.1 to 0.5 per cent – after all, modern packaging lines are highly automated. The scientific data, however, paint a far less flattering picture.

    The well-known market study by OFI in Vienna

    A comprehensive investigation by the Austrian Research Institute for Chemistry and Technology (OFI) in Vienna (led by Dr. Michael Washüttl, Prof. Manfred Tacker and Birgit Tauschitz) is particularly revealing in this respect. In the German-speaking region (D-A-CH), OFI examined a total of more than 1,600 foods packed under modified atmosphere (MAP – Modified Atmosphere Packaging) from regular retail – including meat and sausage products, cheese, fish, bakery products and convenience foods. In addition, a specific sample of 386 modified atmosphere packs from German retail was examined in detail.

    The result caused a stir throughout the entire packaging industry:

    • Only 56% of all MAP packs examined had an optimal modified atmosphere at retail.
    • approx. 33% up to as much as 44% of the packs – and in the German retail sample even almost 50% – showed significant deficiencies in the gas mixture or did not fulfil their intended purpose of extending shelf life.
    • Besides an incorrectly designed film barrier and interactions between the packed product and the test gas, the Viennese researchers identified the main causes above all as leaks due to defective seals: unsuitable sealing tools, misadjusted or incorrectly reading temperature sensors on the sealing jaws, mechanical overstressing during packing and product contamination in the seal area.

    Complementary studies by WRAP and IVLV / Fraunhofer IVV

    These findings are fully consistent with other international surveys. A widely cited British study by the organisation WRAP (“Seal integrity and the impact on food waste”, Dudbridge & Turner) and IVLV Information Sheet No. 114 from the research project EVOCOSEAL (Fraunhofer IVV in cooperation with Hasselt University and KU Leuven) show impressively that:

    • In 58% of all cases of defective packaging, contamination of the seal (by product splashes, fats, dusts or condensate) is the primary cause of pack failure.
    • Depending on the film type and contamination, product residues in the seal area can cause seal strength to drop by up to 88%.

    Even though these studies date back a few years, the trend remains unbroken today. Sealing problems are still the main cause of leaks in flexible packaging.

    My practical estimate: How many packs are really affected today?

    Of course, inline quality control has evolved since the first OFI surveys. Obvious “bursts” or completely open seals that are immediately noticed on the filling line are usually in the range of 0.1 to 1% at well-run plants. But that is only half the truth – because a large proportion of critical leaks consist of micro-leaks (capillaries 10 to 50 µm in diameter) at fold transitions or of a pre-damaged hot seal (hot tack), which often go undetected in a quick spot check in a water bath or only open up during transport as a result of pressure and vibration stresses.

    If we combine the findings of OFI Vienna, the Fraunhofer/IVLV research and our ongoing laboratory tests at Innoform Testservice, my realistic estimate for today’s market is as follows:

    • 70 to 80% of all real-world package leaks do not originate in the intact film surface, but directly in or immediately next to the seal (seal edges, gussets, 2-/4-ply transitions).
    • Across all flexible film packaging at retail, an estimated 3 to 8% of all packs have avoidable seal weaknesses or micro-leaks.
    • For sensitive MAP packs, vacuum packs, liquid and powder products, as well as on lines recently converted to mono-materials or paper-based laminates, the rate of seals that are not optimally leak-tight is in practice often as high as 5 to 15%.

    “Barrier begins where leak tightness ends. Before philosophising about permeation, everything has to be tight first.”


    Barrier vs. leak tightness: why a single 25 µm hole renders any high-barrier film package useless

    To understand why even the smallest sealing defects have such dramatic consequences for product protection, it is worth looking at a simple calculation that I regularly work through in our seminar “Leak Testing, Sealing and Processing of Barrier Film Packaging (Barrier Films Part 4 (in German))”.

    Imagine a classic high-barrier pouch with a surface area of 375 cm², made from a metallised laminate (PET-BO met. 12 µm / PE 90 µm). The oxygen transmission rate (OTR) of this intact barrier film is an excellent 0.3 cm³/(m² · d · bar):

    • Oxygen ingress through permeation (intact film area): Across the entire pouch area of 375 cm², with a pure oxygen gradient, only 0.011 cm³ of oxygen per day per pack diffuses through the material.
    • Oxygen ingress through a single micro-leak in the seal: Now let us assume that a tiny crease or a dust particle has created a single continuous capillary (“channel”) with a diameter of just 25 µm (half the thickness of a human hair!) in the 10 mm wide seal. Through this one micro-channel alone, around 0.052 cm³ of gas flows into the pack every day.

    In plain terms: a single 25 µm capillary in the seal lets almost five times as much oxygen into the package as the entire high-barrier film put together! And if the pore diameter is 50 µm, gas ingress multiplies drastically once again. Anyone who spends a lot of money on EVOH, SiOx, AlOx or aluminium barriers but does not have their seals under control is simply throwing money out of the window.

    “How tight is tight?” – Typical defects and leak rates

    Absolute leak tightness in the physical sense does not exist – what matters is always which defect size becomes critical for your specific product. The following overview (based on guide values from the Fraunhofer Institute IVV and leak measurement technology) helps with practical classification:

    Everyday requirementCritical pore size / capillary diameterTypical leak rate (guide value)Practical example & risk
    Sift-proof / insect-proofapprox. 100 – 200 µm> 10⁻¹ mbar·l/sSugar, flour, rice; protection against stored-product pests
    Dust-tightapprox. 25 – 30 µmapprox. 10⁻¹ to 10⁻² mbar·l/sFine powders, spices, cocoa powder
    Water-vapour-tightapprox. 20 – 25 µmapprox. 10⁻² mbar·l/sDry products, crackers, milk powder clumping
    Liquid-tight (droplets)approx. 15 – 20 µmapprox. 10⁻² mbar·l/sSoups, sauces, pet food, wet wipes
    Vapour-tight (“sweating”)approx. 10 – 15 µmapprox. 10⁻³ mbar·l/sAroma loss, drying out during storage
    Gas-tight & bacteria-tightapprox. 5 – 10 µmapprox. 10⁻⁴ mbar·l/sMAP packs, vacuum packs, medical devices

    The 5 typical causes of leaking seals – and how to avoid them

    When customers from the food, pharmaceutical or consumer goods industries send rejected pouches or trays to our laboratory in Oldenburg, our failure analysis repeatedly uncovers five recurring failure patterns. The good news: each and every one of these problems can be reliably eliminated with the right choice of materials and targeted testing.

    Laboratory heat sealer at Innoform Testservice testing seal strength and package integrity of flexible packaging with overview of standards DIN 55529, ASTM F 1921, DIN EN 868-5 and ASTM D 3078
    Systematic root-cause analysis at Innoform Testservice: Combining seal strength curves (DIN 55529), hot-tack testing (ASTM F 1921), dye penetration (DIN EN 868-5) and vacuum leak testing (ASTM D 3078) reliably detects micro-capillaries and gusset defects.

    1. Contamination in the seal area (“sealing through contamination”)

    When pouches and trays are filled, cocoa powder, ground coffee, milk powder or grated cheese gets stirred up; with moist products, marinades, fats, cooking oils or condensation splash onto the seal area. If this product gets between the sealing jaws, it acts as a release layer and prevents the molten polymer chains from interdiffusing (entangling).

    How to avoid this defect: Besides optimised product dosing and extraction, the decisive factor here is above all the sealant layer. While simple standard PE-LD or PP-BO quickly reaches its limits when contaminated, low-melting metallocene polyethylenes (mLLDPE), ethylene copolymers (such as EVA) or ionomers (known e.g. as Surlyn®) can “flow around” dust particles and the finest grease films much better thanks to their low melt viscosity and still seal tightly.

    2. The critical 2-to-4-layer transition (side gussets, overlaps and “gussets”)

    Take a close look at a typical flow wrap pouch (flowpack) or a stand-up pouch (doypack): where the longitudinal seal (fin seal) or the side gusset runs into the cross seal, the material thickness jumps abruptly from two layers to four layers. Precisely at this edge, a small wedge-shaped cavity forms – the so-called gusset.

    If the sealing layer is designed too thin (e.g. only a few micrometres of heat-sealable coex PP) or the sealing jaws are rigid and incorrectly profiled, the volume of molten polymer is simply insufficient to “flood” this step. A continuous capillary channel of 20 to 100 µm remains open.

    How to avoid this defect: The thickness and flowability of the sealing layer must always be matched to the total thickness of the laminate and the step height. Using a microtome cross-section under the light microscope in combination with a dye penetration test according to DIN 55508-2, we can make visible in our laboratory within a very short time whether the gusset is cleanly filled or whether polymer mass is missing.

    3. Insufficient hot seal strength (hot tack failure)

    On high-speed vertical form-fill-seal machines (VFFS), the following happens: the cross jaws seal the bottom seam, open, and just milliseconds later the heavy product (e.g. 500 g of nuts, frozen vegetables or washing powder) drops from the forming tube directly onto the still hot, molten seal. At the same time, the film draw-off pulls on the seal.

    If the sealing layer has too weak a hot tack (hot seal strength) in this hot temperature window, the melt is partially pulled apart. Fine strings, micro-cavities or local tears form. The insidious part: if you later test the cooled pouch in a standard tensile test, the seal still appears to be strong – but due to the micro-channels drawn while hot, the pouch has long since been leaking!

    How to avoid this defect: In high-speed FFS processes, never rely solely on the cold seal strength. Have a complete hot tack curve according to DIN 55571-2 or ASTM F 1921 recorded. It shows exactly at which sealing temperature the material offers the highest resistance in the hot state.

    4. Narrower sealing windows due to mono-materials and paper laminates (PPWR effect)

    In the past, classic laminates such as PET/PE or OPA/PE were extremely forgiving: the outer PET or PA layer only melted beyond 220 to 250 °C, while the inner PE layer already sealed from 105 °C. The machine operator had a comfortable sealing window of 30 to 50 °C. If the seal did not hold, you simply turned up the temperature on the machine by 15 degrees – and it ran.

    With the European Packaging and Packaging Waste Regulation (PPWR) and the switch to recyclable all-PE or all-PP mono-materials as well as to fibre-based barrier papers with ultra-thin dispersion sealing coatings, this picture has completely reversed:

    • With polyolefin mono-materials, the melting points of the outer layer (e.g. oriented BOPE or BOPP) and the inner layer (sealant PE or sealant PP) are close together. If sealing is too hot, the outer film shrinks, the seal warps into waves or the molten polymer is squeezed out at the edge of the sealing jaw – resulting in a thin spot and a classic seal edge fracture.
    • With paper laminates, the paper acts as a thermal insulator (poor heat transfer), while the inner dispersion coating is often only a few grams per square metre thin and can barely compensate for unevenness in the paper fibres.
    Sealing curve from an Innoform test report comparing two film samples
    Example from an Innoform test report: comparing the sealing curves of two film batches (sample 1 vs. sample 2) immediately reveals whether the seal initiation temperature (SIT) has shifted upwards by 10 to 15 °C.

    How to avoid this defect: As the diagram from one of our sample laboratory reports shows, even a slight change in the coextrusion formulation (e.g. a lower proportion of low-melting plastomer in the PE blend) can shift the seal initiation temperature (SIT) upwards by 10 to 15 °C. By combining a laboratory sealing curve (DIN 55529), DSC melting point analysis and FTIR spectroscopy, we determine beyond doubt whether the material has deviated or whether the temperature distribution of your sealing jaws needs to be readjusted.

    5. The trade-off between leak tightness and easy opening (peel seals)

    Consumers want packaging that can be opened smoothly by hand without scissors (easy peel) – while quality assurance demands absolute leak tightness throughout the entire logistics chain. A widespread misconception is: “A peel seal with 4 N/15 mm is less tight than a lock seal with 40 N/15 mm.”

    Physically, this is not true: as long as the sealing layer is continuously sealed through, a peel seal (whether adhesive peel, cohesive peel via incompatible blends such as polybutene-1, or delamination peel) is just as gas- and liquid-tight as a lock seal. It only becomes critical when external forces – such as the post-tensioning of a vacuum pack, the rise in internal pressure during lorry transport over an Alpine pass, or impacts inside the carton – exceed the peel initiation force of the seal and the seal partially “creeps open”.

    How to avoid this defect: In addition to the pure strip tensile force, also test the actual opening forces on the complete package according to DIN 55409-1 (flexible packaging) or DIN 55409-2 (rigid trays), and specifically match the sealing jaw contour (e.g. a rounded profile for gentle peel initiation) to your peel system.


    Testing correctly at Innoform Testservice: systematically safeguarding seal strength and leak tightness

    In our test laboratory in Oldenburg, accredited to DIN EN ISO/IEC 17025 (DAkkS), we make a strict distinction between two complementary testing pillars: mechanical seal tests (How high is the holding force and how wide is the process window?) and physical leak tightness tests (Are there any continuous channels or pores?). Both are inseparable parts of a sound packaging specification.

    Pillar 1: Testing seal strength, sealing curves and hot tack

    In the mechanical testing of seals, a specimen strip exactly 15 mm wide is die-cut perpendicular to the seal and pulled apart in the tensile testing machine at a defined speed. But be careful: anyone who looks only at the bare figure in N/15 mm in the test report often overlooks the most important information!

    “Force values alone are not enough – the failure pattern tells the truth.”

    That is why, at Innoform, we always document the tear or failure pattern for every seal strength measurement:

    • Clean peel (separation of the sealant layer): Desirable for easy-opening packaging; for permanent seals, however, it indicates a sealing temperature that is too low (cold seal).
    • Break directly at the seal edge (seal edge failure): A typical sign of excessive sealing temperature or sealing pressure – the sealant layer has been squeezed and weakened at the edge of the jaw.
    • Delamination of the laminate: The seal is stronger than the lamination between the individual layers – the film splits within the laminate (an indication of insufficient bond strength or an unsuitable laminating adhesive).
    • Elongation / break in the free film strip: The seal is stronger than the base material itself (a true weld seal).
    Test method at Innoform TestserviceStandard / basisMeasured variable & temperature rangeTypical practical benefit
    Seal strength (strip tensile test)DIN 55529, ASTM F 88 / F 88M, DIN EN 868-5 Annex DMaximum force / force curve in N/15 mm (-40 °C to +120 °C) incl. failure patternQuality control of finished pouches, medical packaging & trays; testing under deep-freeze or pasteurisation conditions
    Sealing curves on the laboratory heat sealerDIN 55529, ASTM F 88Seal strength as a function of temperature, time & pressure (e.g. 80 – 220 °C)Determination of seal initiation temperature (SIT) and optimum sealing window; comparison of new mono-materials with reference films
    Hot tack testDIN 55571-2, ASTM F 1921Maximum holding force of the still-hot seal in N/15 mm immediately after the jaws openIndispensable for high-speed VFFS and HFFS flow-wrap machines as well as heavy, free-flowing or frozen products
    Opening forces of peelable packsDIN 55409-1 (flexible), DIN 55409-2 (rigid)Initial peel force and continued peel force in N on the original packPractical assessment of opening behaviour (easy opening) from the consumer’s perspective
    Seal quality of PE sacks & paperDIN 55529, GKV test sheets I–IV, DIN EN 868-4Seal strength, fibre tear & seal qualitySafeguarding heavy-duty sacks, industrial bags and sterilisable paper/film packaging

    Pillar 2: Overview of leak tightness tests and leak detection

    A high seal strength in the strip tensile test does not prove that no hair-fine capillary has remained open in the 2-/4-layer gusset area. That is why, within our seal strength & leak tightness testing services, we combine strength testing with targeted leak detection and leak tightness tests:

    Leak tightness / leak test methodStandard / test specificationDetection limit (approx.)Principle & ideal application
    Tracer gas method (forming gas N₂/H₂)IVLV Information Sheet No. 102< 10 µm (gas-tight)Filling with a hydrogen/nitrogen mixture and highly sensitive H₂ sniffer probe; non-destructive localisation of the smallest gas leaks in MAP and vacuum packs
    Dye method with methylene blueDIN 55508-2approx. 10 – 20 µmAn alcohol solution with low surface tension creeps into even the finest seal capillaries and gussets and stains defects a high-contrast blue
    Dye penetration test (rhodamine B / aqueous)ASTM F 1929approx. 15 – 50 µmInternational standard (especially pharma/medical) for detecting channels in transparent and opaque seals
    Penetrating oil test & original product testIn-house method PV036approx. 10 – 20 µmSpecial test for oily and fatty products and for detecting the finest pores (pinholes) after flex stress (Gelbo Flex)
    Vacuum chamber / water bath (bubble test)Standard laboratory method (DIN EN ISO 11607 / ASTM D 3078)approx. 15 – 30 µmThe sealed pack is submerged under a defined vacuum; escaping gas bubbles immediately reveal the exact location of the leak
    Light table & copper depositionDIN EN 546-4, FhG Information Sheet 29 Part 1from 20 µm (optical) or micro-pinholesTesting of aluminium foils and aluminium laminates for pores, flex cracks and corrosion defects

    Practical checklist: How to permanently eliminate complaints caused by poor seals

    From our day-to-day consulting work, five specific rules have proven effective in helping film manufacturers, converters and packers drastically reduce their failure rates:

    1. Specify performance, not just film thicknesses: Make the seal initiation temperature (SIT), the sealing window in °C, the required seal strength in N/15 mm (including the desired failure mode!) and, for high-speed flow-wrap processes, the minimum hot tack binding requirements in your film specification.
    2. Retain reference samples systematically: Set aside an unprinted or unsealed reference sample from a film batch that has demonstrably run perfectly. If machine problems occur later, a direct laboratory comparison of good and bad samples can clarify within a few days what has changed.
    3. Test in the laboratory before switching to mono-materials: Do not take new all-PE, all-PP or paper-based laminates onto the production line “flying blind”. A sealing curve and hot tack curve recorded in the laboratory beforehand saves costly machine downtime and tonnes of waste.
    4. Check sealing jaws regularly by thermography and mechanical testing: As the OFI study already showed, the digital display on the control cabinet often does not match the actual surface temperature of the sealing jaw. Check the temperature profile and pressure distribution regularly (e.g. using carbon paper or pressure-indicating film imprints), especially in the area of the 2-to-4-layer transition.
    5. Test leak tightness with the right method: Briefly squeezing the pouch by hand or a non-specific water bath test is often not sufficient for MAP and high-barrier packs. For critical products, use dye penetration testing to DIN 55508-2 or the tracer gas method according to IVLV Guideline 102.

    Knowledge prevents failure costs: Our relevant Innoform seminars

    Good test results only deliver their full benefit when purchasing, quality assurance, packaging development and machine operators speak the same technical language. If you and your team would like to delve deeper into the relationships between polymer structure, sealing technology and test methodology, I recommend our practice-oriented web seminars and courses at Innoform Coaching:


    Frequently asked questions on seal strength and leak testing (FAQ)

    Why does a package sometimes leak despite high seal strength in N/15 mm?

    Seal strength according to DIN 55529 or ASTM F 88 measures the mechanical holding force on a 15 mm wide strip of the cooled seal. Leaks, however, often occur at isolated points – for example through a fine capillary (10–30 µm) at the 2-to-4-layer transition (side fold/gusset), through individual product particles in the seal, or through brief opening of the still-hot seal due to insufficient hot seal strength (hot tack). Strength testing should therefore always be supplemented by targeted leak testing (e.g. methylene blue test to DIN 55508-2 or tracer gas test).

    According to studies, how many modified atmosphere packs (MAP) in retail are defective?

    In the well-known market study by the Austrian Research Institute for Chemistry and Technology (OFI) in Vienna covering more than 1,600 MAP packs in the German-speaking region, only 56 % had an optimal modified atmosphere; around one third to 44 % (and almost 50 % in a German retail sample of 386 packs) showed defects. Supplementary studies (WRAP, Fraunhofer IVV / IVLV Guideline 114) show that in 58 % of defective packs a contaminated seal is the main cause. In current practice, it can be assumed that 70 to 80 % of all genuine package leaks are located in or directly adjacent to the seal.

    Which test method detects even the smallest micro-leaks in seals?

    For directly visualising very fine channels in the seal from approx. 10–20 µm, dye penetration testing with methylene blue solution to DIN 55508-2 (or ASTM F 1929 with aqueous dye solution) is ideally suited. If closed packs are to be tested non-destructively for gas tightness (defects < 10 µm), the tracer gas method using forming gas (hydrogen/nitrogen) and a sensitive hydrogen sensor in accordance with IVLV Guideline No. 102 is the method of choice.

    When should a hot tack test be carried out in addition to the sealing curve?

    A hot tack test according to DIN 55571-2 or ASTM F 1921 is indispensable whenever the seal is subjected to mechanical stress while it is still hot and not yet fully cooled. This applies above all to high-speed vertical and horizontal form-fill-seal machines (v-FFS / h-FFS), heavy or sharp-edged products, and the switch from conventional PET/PE laminates to mono-materials (PE, PP) or barrier papers.


    My conclusion: when damage occurs, let the analysis do the talking!

    Leaking packs are not an unavoidable fate – and certainly no reason for weeks of finger-pointing between film supplier and packer. Whether a seal fails because of product contamination, a sealing window that is too narrow with the new mono-material, insufficient hot tack or an open gusset at the 2-/4-layer transition can now be clarified in the laboratory quickly, objectively and in compliance with standards.

    My advice from practice is therefore: Specify rather than speculate. And if things do get stuck on the line, or packs start drawing air at retail: don’t blindly adjust the sealing temperature – send your good and bad samples to our laboratory in Oldenburg instead. We test seal strength and leak tightness under accreditation, all from a single source, and deliver results that let you get production running reliably again straight away.

    Yours, Karsten Schröder
    Innoform Testservice – your accredited test laboratory for flexible packaging

    Sources and references (technical literature, studies & test standards)

    • Österreichisches Forschungsinstitut für Chemie und Technik (OFI), Vienna; Washüttl, M., Tacker, M., Tauschitz, B.: Market studies on the quality of food packed under modified atmosphere (MAP) in German-speaking retail (examination of more than 1,600 MAP packs in Germany, Austria and Switzerland and 386 packs in German food retail).
    • WRAP (Waste & Resources Action Programme), UK; Dudbridge, M., Turner, R. (University of Lincoln): Seal Integrity and the Impact on Food Waste – study of leakage causes and contamination in the seal area.
    • Industrievereinigung für Lebensmitteltechnologie und Verpackung e. V. (IVLV) / Fraunhofer Institute for Process Engineering and Packaging (IVV), Freising (in cooperation with Universiteit Hasselt & KU Leuven): IVLV Technical Leaflet No. 114 (research project EVOCOSEAL – influence of product contamination in the seal area on seal quality) and IVLV Technical Leaflet No. 102 (tracer gas method for leak testing of packaging using forming gas N₂/H₂).
    • DIN 55529: Packaging – Determination of the seal strength of seals made from flexible packaging materials (strip tensile test and assessment of the failure pattern).
    • ASTM F 88 / F 88M: Standard Test Method for Seal Strength of Flexible Barrier Materials.
    • DIN 55571-2 and ASTM F 1921 / F 1921M: Determination of hot seal strength (hot tack) of heat-sealable thermoplastic polymers and flexible barrier materials immediately after the sealing process.
    • DIN 55508-2: Testing of packaging – Leak testing of flexible packaging, Part 2: Dye method (methylene blue solution); supplemented by DIN EN 868-5 and ASTM F 1929 (Standard Test Method for Detecting Seal Leaks in Porous Medical Packaging by Dye Penetration).
    • DIN 55409-1 and DIN 55409-2: Testing of packaging – Determination of the opening forces of peelable packaging (Part 1: Flexible packaging; Part 2: Rigid packaging/trays).
    • ASTM D 3078: Standard Test Method for Determination of Leaks in Flexible Packaging by Bubble Emission (vacuum chamber water bath test) and DIN EN ISO 11607-1.
    • DIN EN 546-4 and Fraunhofer Technical Leaflet No. 29 Sheet 1: Testing of aluminium foils and aluminium composite films for pores (pinholes) and flex cracks using a light table and electrolytic copper deposition.
    • Schröder, K.: Seminar documents “Leak Testing, Sealing and Processing of Barrier Film Packaging (Barrier Films Part 4 – BVd)” and “Fundamentals of Packaging Films”, Innoform Coaching / Innoform Testservice, Oldenburg.
  • Understanding the fat barrier of fibre-based packaging – why testing is crucial

    Understanding the fat barrier of fibre-based packaging – why testing is crucial

    Fatty foods pose particular challenges for packaging. Fats can penetrate materials, affect their appearance or cause problems from the very first contact. This is precisely why tests such as fat resistance, fat permeability and fat repellency play a central role – both in development and in quality assurance. 

    In this context, two fundamental perspectives can be distinguished: 

    • Barrier effect (fat resistance & fat permeability) → Behaviour within the material 
    • Fat repellency (lipophobia) → Behaviour on the surface  

    It is only the combination of these two approaches that allows for a realistic assessment. 

    Fat resistance and fat permeability: the barrier is the deciding factor in the long term.

    Together, fat resistance and oil permeability describe a material’s ability to retain oil and limit its passage.

    • Fat permeability indicates how easily and how quickly fat migrates through a material  
    • Fat tightness answers the question of whether this barrier is sufficient for the application  

    Why is this relevant? 

    In practical use, the main focus is on the long-term effect: 

    • Protection of the product throughout its entire storage period 
    • Prevention of grease migration and structural material failure
    • Ensuring the functional properties of the packaging 

    Key question: 
    Does the material reliably repel fat? 

    Oil repellency (KIT test) – the surface is the first point of contact

    Fat repellency describes the behaviour of fat on the surface of the material. 

    • Fat can either be rejected or 
    • it wets and penetrates  

    The KIT test provides a standardised assessment of this via a parameter (KIT level). 

    Why is this relevant? 

    The user interface often determines the first impression and short-term performance:

    • Preventing visible fat stains 
    • Impact on consumer perception
    • Protection against initial wetting and the resulting penetration

    Key question: 
    What happens when fat first comes into contact with the packaging? 

    Structure vs. surface – two sides of the same coin

    Property Fat tightness & permeability Fat repellency (KIT) 
    Focus Material structureSurface 
    Statement Migration patternsWetting resistance
    Time horizonLong-term reviewQuick test
    Meaning Functional barrierAppearance & First impression 

    Why both tests are necessary in practice

    A high KIT value alone does not guarantee high fat density. Fat behaviour is always the result of several factors – and that is precisely why it is so important to consider them together:

    • Good fat repellency can delay grease from sticking, but it cannot replace a barrier
    • Good barrier properties delay penetration, but do not necessarily prevent staining
    • Materials – particularly paper-based ones – often exhibit time-dependent behaviour  

    Typical practical implications 

    • Complaints: visible fat stains despite adequate protection
    • Quality issues: Fatting during prolonged storage, Sensory impairment
    • Process disruptions: Fat affects sealing, adhesion, mechanical stability or handling  

    This interaction is becoming increasingly important, particularly in the context of sustainable packaging solutions (e. g. paper-based systems).

    Classification by application 

    • Product development: 
      A combination of barrier assessment and surface analysis  
    • Quality assurance: 
      Clear requirements regarding grease density, supplemented by KIT values  
    • Material optimisation: 
      Targeted adaptation of coatings and structures  

    Conclusion

    The assessment of fat behaviour can be boiled down to two key questions: 

    • What happens within the material? → Oil resistance & oil permeability  
    • What happens on the surface? → Fat repellency  

    These two aspects are inextricably linked. Only by considering them together can we develop packaging that is both functional and visually appealing – from the very first encounter through to long-term use. 

  • Particle and Foreign Body Analysis

    Particle and Foreign Body Analysis

    Precise Characterization for Quality, Safety and Root Cause Clarification

    Particles and unwanted foreign bodies represent a significant quality and risk potential in the manufacture and processing of flexible packaging. Especially with polymer-based materials, multi-layer systems or functional coatings, even the smallest contaminations lead to functional failures, optical impairments or regulatory complaints. The systematic analysis of such anomalies is therefore a central component of modern quality assurance and damage investigation along the entire value chain.

    Definition: Particle vs. Foreign Body Analysis

    Particle analysis examines the size, shape, number and material properties of the smallest particles on or within a product. Foreign body analysis goes beyond this: it identifies substances that do not belong to the intended material composition. The goal is to clearly characterize the nature of the particles and precisely determine their origin. On this basis, causes can be narrowed down, process steps optimized and future deviations avoided.

    Systematic Microscopy at Innoform

    At Innoform, particle and foreign body analyses are performed using high-quality light microscopy systems that enable differentiated assessment. Each examination begins with systematic image documentation. First, overview images are created to capture the position, distribution and embedding situation of the anomaly in the overall context. This is followed by detailed microscopic examination at higher magnification. This two-stage approach ensures both classification within the sample matrix and precise analysis of morphological details.

    Preparation of Composite Materials and Cross-Sections

    Special importance is attached to sample preparation. If particles are enclosed in the matrix – for example in a plastic film, a coating or a complex composite material – the production of a cross-section is often required. Through targeted cutting technique or micromechanical preparation, the embedding situation is exposed. Interfaces, adhesion states and possible interactions between matrix and foreign body become assessable. Especially with multi-layer systems, the cross-section provides valuable indications of which process stage (e.g. extrusion or lamination) a contamination was introduced.

    Foreign bodies in flexible packaging and coatings
    Microscopic image of a foreign body

    Material Identification by Means of IR Spectroscopy

    Morphological examination is often only the first step. For identification of material composition, we use among other methods infrared spectroscopy (IR). It allows the determination of molecular structures based on characteristic vibrational bands. Innoform uses IR analytics in both reflectance and transmission mode. The choice of technique depends on the nature and transparency of the particle. By comparison with reference databases, organic materials – such as polymers, adhesives, coating components or external contaminations – can be clearly identified.

    Complementary Methods: Raman and Thermal Analysis

    In addition, Raman spectroscopy can be used. It offers high lateral resolution for the smallest particles and often allows analysis directly in the embedded state. The combination of IR and Raman spectroscopy significantly increases identification reliability. In special cases, thermal methods such as differential scanning calorimetry (DSC) provide additional insights into melting behavior or thermal stability. This is particularly helpful with polymeric foreign bodies to distinguish materials from one another or to obtain indications of additives.

    Conclusion: Process Safety for Converters and Fillers

    The strength of a well-founded analysis lies in the systematic combination of all information. Morphology, chemistry and thermal behavior yield a coherent overall picture. This enables conclusions about potential sources of entry – such as abrasion from machine components, contaminations from raw materials or residues from cleaning processes. This offers companies decisive advantages: complaints can be objectively evaluated and regulatory requirements, for example for food contact materials, can be reliably documented. Professional analytics is thus an indispensable instrument for securing product integrity.

  • The Most Important Testing Methods for Flexible Packaging – Explained in Practical Terms

    The Most Important Testing Methods for Flexible Packaging – Explained in Practical Terms

    Flexible packaging is often considered simple plastic products – in reality, films are among the most challenging materials of all. Their behavior is shaped not only by the material itself, but at least as much by the manufacturing process. At Innoform Testservice, we see daily how important the correct selection and interpretation of testing methods is.

    The web seminar “Fundamentals of Testing Methods Part C“ impressively demonstrated that film testing is not an academic exercise, but the foundation for functional, safe, and recyclable packaging. This article summarizes the most important findings – concise, practical, and with personal commentary.


    1. Basic Tests: What Every Film Reveals

    Density – Key Parameter for Recycling, Strength & Barrier

    Density influences not only mechanical properties but also behavior in the recycling process.

    • Polyolefins (PE, PP) float – therefore visible in oceans
    • PET, PA, PVC sink – therefore “invisible” portion on the ocean floor
    • Higher PE density = higher strength, better barrier
    • Lower density = better sealability and more

    Practice:

    “When an extruder speaks of 45 density, they mean 0.945 – and immediately know how the raw material will behave.”


    Basis Weight – Fast, Robust, Practical

    One of the simplest methods, especially for:

    • Incoming inspection
    • Adhesive application quantities
    • Adhesive application testing for laminated films

    With a circle cutter and analytical balance, differences can be tracked excellently.


    Film Thickness – Often Overestimated

    Thickness is specified everywhere but is rarely decisive for function.
    Problem: Measurement errors due to different probe heads and methods are enormous.
    More important are:

    • mechanical values
    • shrinkage
    • flatness
    • barriers

    Practice quote:

    “For most properties, we don’t actually need the thickness.” One should only specify what is really needed and wanted – namely performance properties.


    2. Flatness & Curl – Underestimated Practical Parameters

    Flatness determines whether a film functions on the machine.
    Typical causes of poor flatness:

    • incorrect web tension during lamination
    • moisture absorption in PA-containing laminates
    • bimetal effects in multi-material laminates
    • winding errors (too tight on core, too loose outside)

    Easy to measure:

    • punch out circles
    • condition
    • place on table
    • measure curl height

    Practical benefit:

    • Quickly recognizable whether a batch was produced cleanly
    • Ideal for goods receiving to evaluate runnability on machines

    3. Shrinkage Testing – Important for Sleeves, Hoods & Thermoforming Applications

    Film “remembers” the stretching from the production process.
    Measured are:

    • Shrinkage
    • Shrink force

    Relevant applications:

    • Pallet hoods
    • Full-body sleeves
    • Thermoformed packaging

    Practice tip:

    “Shrinkage and shrink force are two different tests – and both can be crucial.”


    4. Tensile Test – The Technically Most Common but Error-Prone Test

    The tensile test is the central mechanical test – but also extremely sensitive.
    It provides among others:

    • Tensile strength
    • Elongation at break
    • Tear propagation resistance
    • Secant modulus

    What Really Matters in Practice:

    1. Sample Preparation

    Notches and inaccurate widths ruin every value.
    → Always work with specimen cutters or cutting dies.

    2. The Right Grips

    Flat-convex grips prevent slipping of the material.
    → Especially important for soft PE films.

    3. Gauge Length & Speed

    Deviations from standards often explain differing supplier values.
    → Always compare: lengths, speeds, grips.


    Secant Modulus – The Practical Value Par Excellence

    It measures stiffness at low elongation (<1%) – and thus determines runnability on machines. This property is also called tensile stiffness

    Example:

    • Too stiff → Multivac cannot manage re-tensioning
    • Too soft (e.g., mono-material films) → machine must adjust web tension

    Practice quote:

    “The secant modulus is the most important parameter for printers, laminators, and packers regarding tensile stress”


    5. Seal Strength Testing & Hot-Tack – Package Safety

    Seal Strength

    Shows how stable the pouch remains.
    Important: Document failure modes!
    Possible error causes directly visible:

    • Layer tear-off
    • Delamination
    • Weak inner layer
    • Incorrectly treated surface

    Karsten:

    “Force values alone are insufficient – the failure mode tells the truth.”


    Hot-Tack

    Indispensable for fast V-FFS machines or frozen products.
    Measures strength of the hot seal immediately after sealing.


    6. Lamination Bond Strength – Quality Assurance for Laminates

    Tested in 180° peel.
    Typical values:

    • good laminates > 5 N (application-dependent)
    • Metallization frequently 1–3 N

    Interpretation of the curve progression provides indications of adhesive curing and layer failure.


    7. Coefficient of Friction (COF) – Decisive for Process Stability

    Two values:

    • µS – static: important for pallet stability
    • µD – dynamic: important for packaging machines (low = good)

    Practical observation:
    Machine malfunctions can often be traced back to incorrect COF values. Unfortunately, laboratory values correlate too little with practice due to slow test speeds.


    8. Optical Tests & Surface Tension

    Haze, Gloss, Transparency

    Decisive for product visibility and marketing.

    Surface Tension (Dyne Value)

    Relevant thresholds:

    • < 34 dyne → poor wetting
    • ≥ 38 dyne → well printable / laminatable

    Practice anecdote:

    “We used to make PE surfboards faster with the Bunsen burner – simply by increasing the surface tension.”


    9. Permeation – Understanding Barrier Properly

    OTR (oxygen transmission rate) and WVTR (water vapor transmission rate) are standard.
    Note:

    • EVOH loses barrier properties with moisture
    • Package tests are more realistic than pure film tests
    • Always specify climate parameters exactly

    Practice recommendation:

    “Calculate first, then test – equipment is expensive, but pre-selection saves time and money.”


    Conclusion

    Flexible packaging is more complex than it appears. The right testing methodology – properly applied, sensibly specified, and correctly interpreted – is the foundation for functional, safe, and sustainable packaging.

    Many of the described methods can be easily integrated into daily operations. The only important thing is to read the results correctly. This practical interpretation is precisely the goal of our seminars and the Innoform Testservice.

  • Labeling Requirements

    Labeling Requirements

    EU Packaging Regulation (PPWR): Labeling Requirement 

    Part 2: What needs to be done now 

    Physical labeling requirements 

    With the EU Packaging Regulation 2025/40 (PPWR), uniform labeling requirements will come into force from August 2028. Packaging must then clearly display information on the type of material, substances of concern, reusability and – where applicable – the recycled content. This information should be provided via standardized pictograms and be understandable throughout Europe. The aim is to provide consumers with simple guidance for proper disposal while ensuring traceability and transparency along the supply chain. 

    Digital information requirements 

    In addition to visible labeling, PPWR requires digital access to additional packaging data – for example via a QR code on the packaging. This so-called digital product passport should provide information on material composition, reusability, recycling instructions and, where applicable, return options. Information that cannot be fully displayed on the packaging due to space constraints can also be stored digitally. Companies must systematically record, maintain and make the relevant data accessible – an important prerequisite for compliance, transparency and efficient product communication. 

    Timeline and recommended action 

    The regulation comes into force in August 2026, with mandatory labeling requirements from August 2028. From 2030, additional labeling of packaging containing substances of concern will be necessary. For packaging manufacturers and packers this means:

    Processes and layouts should be reviewed and adapted now. This includes sufficient space for labeling elements, the integration of IT systems for data management and the training of relevant teams. Those who start implementation early not only ensure compliance with the requirements, but also strategically position themselves for future circular economy requirements. 

    More information also in our web seminars prepared in compact form for flexible packaging converters.

    And we recorded the conversation on the same topic at Fachpack25: https://inno-talk.de/digitalisierung-trifft-recyclingfaehigkeit-bei-wipak/

  • Precise Material Analysis of (Composite) Films

    Precise Material Analysis of (Composite) Films

    Dr. Daniel Wachtendorf 
     
    The material characterization of films plays a crucial role in research and industry, particularly in the development and quality assurance of packaging materials, technical films and composite materials. Various proven methods are used to precisely analyze the structure, composition and thermal properties of these materials. 

    The precise analysis of composite films is essential to understand their structure and properties. They are often used to clarify the following questions:

    1. Material information: How is the film structured? This question is particularly relevant when the material is unknown – for example, to assess recyclability. 
    1. Avoid confusion: Does the delivered film actually correspond to the ordered specification? 
    1. Error detection in the formulation: Is there a deviation or mix-up in the composition? 
    1. Competitive analysis: Which film variants exist on the market – including those from competitors – for specific applications? 

    The Innoform Testservice in Oldenburg offers a comprehensive analysis package for precise determination of film structure and material composition. This includes microtome cross-sections, DSC (Differential Scanning Calorimetry), polarization thermomicroscopy and infrared (IR) spectroscopy. With these methods, well-founded findings can be obtained that are indispensable for quality assurance, product development and market analyses. 

    The first step in analysis 

    When the customer sample is received, we first create a quick microtome cross-section. This provides an initial overview of the complexity of the sample and serves as a basis for planning further investigations. After we have determined the required analysis effort, we prepare a detailed microtome cross-section and usually examine it under high magnification in transmitted light. This method allows the number of layers, their thicknesses and basic structure to be determined exactly.

    The microtome cross-section of a film 

    The images created serve not only as guidance for further analyses, but also for clear visualization for the client. Modern microscopes deliver excellent results and are an essential prerequisite for subsequent material characterization. The microtome cross-section thus forms a central component of the analysis and, together with the tabular summary of results, represents the centerpiece of our reports. 

    Thermal Analysis 

    The second step is Differential Scanning Calorimetry (DSC), a precise method for thermal analysis of the sample. However, before beginning this investigation, halogens must be excluded. This is done using the Beilstein test, a simple chemical detection method for halogens such as PVC or PVDC. We use the property that halogens produce characteristic green flame colorations in the presence of copper. If the film contains halogens, we subsequently forgo DSC analysis to protect the sensor from the resulting gases.

    If the Beilstein test is negative, a thermogram of the sample is created. This provides important thermal parameters such as melting temperatures, melting enthalpies (energy absorption or release) as well as crystallinity and glass transition temperatures. Although DSC does not provide layer-specific results, it offers a comprehensive overview of the thermal properties of the entire sample. Particularly in combination with hot stage microscopy, typical materials such as polyethylene (PE) can be precisely identified. 

    Analysis of the Melting Behavior of Individual Layers 

    Another important step in material characterization is hot stage microscopy. This enables detailed investigation of the melting behavior of individual layers of composite films. After preparing a microtome cross-section, the sample is positioned without medium on a glass slide in the transmitted light microscope. There it is gradually heated in a kind of “mini-oven” and continuously observed. 

    Special polarization filters create a dark field in which semi-crystalline layers become visible as bright areas. Through controlled temperature increase, the melting ranges can be precisely determined. When the melting point is reached, the birefringence disappears, causing the previously bright layers to appear dark. This method allows the thermal properties of individual layers to be accurately determined – even with colored layers, for example with TiO₂, which present a particular challenge. 

    Chemical Analysis of Composition 

    To complement the thermal analyses, infrared (IR) spectroscopy is used. This method provides detailed chemical information about the composition of the individual layers. First, the outer layers of the sample are examined using ATR (attenuated total reflectance) spectroscopy. We then prepare a microtome cross-section and place it in a specially developed stainless steel holder for transmitted light measurement.

    Using an infrared spectrometer, spectra of the individual layers can be recorded and compared with reference spectra. This investigation complements the thermal analyses and serves as a second verification of the results. 

    The intermediate layers of a sample can also be analyzed using the IR microscope, resulting in a complete and detailed structure of the composite film. 

    Summary of investigation results of a film

    Conclusion: Comprehensive Characterization Through Combined Analyses 

    Through the combination of mechanical, thermal and chemical analyses, the analysis package from Innoform Testservice offers an opportunity to characterize films in detail. From the first microtome cross-section to the final IR spectroscopy, a comprehensive picture of the material structure and composition emerges. This precise approach not only provides valuable insights for technical and industrial applications, but also sets a high standard in modern film characterization. 

  • Guidelines on the use of recyclates in food packaging

    Guidelines on the use of recyclates in food packaging

    Associations are pushing for the release of recyclates in direct contact with food. Supposedly, about 42 % of all plastic packagings are intended for food packaging. And therefore the effect of a CO2 reduction by the use of recyclates for food packaging is necessary.

    EU-wide, new rules for the use of recycled plastics in contact with food, e.g. food packaging, will apply from 10 October 2022. Although certain transitional periods still apply until mid-2023, many plastics recyclers and processors must already prepare for the new regulations. Joint guidelines published today by the associations of the plastics processing industry (GKV and its supporting associations) and the plastics recyclers (BDE, bvse) will help them to do so.

    The use of recycled plastics represents an important contribution on the way to a climate-neutral circular economy, because it reduces CO2 emissions in product manufacturing and dependence on fossil raw materials. Recyclates are already irreplaceable for products that come into contact with food, e. g. PET beverage bottles, and they are becoming increasingly important, explains Dr Andreas Bruckschen, Deputy Chief Executive of BDE e.V.

    With the guidelines, plastics associations want to facilitate the application of the new regulations for plastics recyclers and processors and show ways and means of implementing the regulations, some of which are very complicated, explains Herbert Snell, Vice President of the Plastics Recycling Association in the bvse. Together, the three associations appeal to the EU Commission to implement its announcement and finally approve the PET recycling processes that have meanwhile been assessed as safe and thus create legal certainty for the industry.

    The brochure can be downloaded free of charge from the associations’ websites.

    Contacts for queries:

    Dr. Martin Engelmann, m.engelmann@kunststoffverpackungen.de, Tel.: 06172-9266 76,